A welded chair frame comes out of the jig twisted, and the jig was straight. Heat goes in on one side of the section and pulls the tube towards it.
Weld metal shrinks as it cools, and it shrinks towards the weld. 1.2–1.5 mm wall tube, 360° fillet, ground before powder. Every fillet pulls its two parts together by roughly 1 mm per 100 mm of weld length.
On a chair frame with 16 welds, that is a millimetre here and a millimetre there, and the legs end up 3 mm out of plane. You see it as a chair that rocks on a flat floor.
Weld sequence. Opposite welds, alternating, so one pull cancels the next. Welding all four corners of one side first is the fastest way to a twisted frame.
Fixture stiffness. Flex in the jig lets the frame move while it cools. 1.2–1.5 mm tube in a light jig pulls the jig, not the frame.
Heat input. Lower current, faster travel, shorter fillets. Four millimetres of fillet on a 1.5 mm wall burns through and adds distortion without adding strength.
Straightening after. Press and check on a flat table, done cold, before powder coat. Not after — powder hides nothing and a bent frame with fresh paint is scrap.
Stacking chairs are the strictest case. Eight chairs in a stack transmit every error upward, and a 3 mm twist at the bottom becomes a stack that leans. Users notice a leaning stack immediately.
For stacking frames, specify a post-weld check on a flat plate with a 1.5 mm feeler gauge. If the frame rocks, it goes back to be straightened before it is painted.
Set a chair on a granite or glass surface and push each corner. Movement means the frame is out of plane. Then measure the diagonal between opposite leg feet — more than 2 mm difference between the two diagonals is a twisted frame.
Weld quality is the other half of the story, covered in weld quality on a chair frame. Prep before coating sits in powder coat prep.
Send the floor plan and the seat count. Quote and finish chip in one reply.
Start a conversation →