A pin meter, ten minutes and a notebook settle most timber arguments before they start. The number to compare against is on the packing list.
Pin meters read the top 20 mm. On a 60 mm rail the surface can be two points drier than the core, which is why a reading taken on a sunny loading dock looks better than the timber is. Take the reading on a freshly cut face or on an end that has been planed.
Pin meter on 20% of the batch, cut test on one piece per kiln charge. We pack at 8–10% at packing and record the figure per kiln charge, so the buyer has something to compare with.
Ten chairs out of a delivery, three readings each: one on a front leg, one on a seat rail, one on a back post. Log the average and the spread. Spread of four points inside one container means the kiln charge was mixed, which matters more than the average.
Then the same on a table top if there is one, at the centre and 50 mm from the edge. Tops move twice as much as they need to when the centre and the edge disagree.
Timber at 9% going into a room held at 45% relative humidity will gain moisture and swell. That is fine — joints close, nothing cracks. Timber at 9% going into a room at 22% relative humidity will lose moisture and shrink, and shrinkage is what opens joints.
Ask what the seasonal humidity of the dining room is before the order, not after. The answer changes the packing target by two points, which is the difference between a frame that stays tight and one that clicks in February.
Do not unpack. Keep the cartons closed in the room for 72 hours and read again. Most high readings are surface moisture from a humid port, and they fall without anyone doing anything.
If the core is still high after three days, log it and photograph the meter. Claims made with a reading and a date go somewhere; claims made three months later do not. The moisture table sits in the timber guide, and moisture content at packing covers the factory side.
Send the floor plan and the seat count. Quote and finish chip in one reply.
Start a conversation →